Reading the 20CrMo Designation Before Ordering Tube
The name 20CrMo is a Chinese alloy structural steel designation that carries three pieces of information in six characters: a nominal carbon content, a chromium addition and a molybdenum addition. The leading figure 20 means a nominal carbon content of about 0.20 percent, expressed in hundredths of a percent, and the two element symbols record chromium and molybdenum without a trailing multiplier because both are present at average levels below 1.5 percent. A purchaser who understands that structure can read the chemistry before opening a mill certificate, and can spot a mis-declared heat immediately: a 40Cr tube and a 20CrMo tube look identical on the rack but are heat treated and used very differently.
20CrMo is a low-carbon, chromium-molybdenum case-hardening and quench-and-temper grade. The low carbon keeps the core tough and permits carburising to a hard case, while chromium improves hardenability and wear resistance and molybdenum suppresses temper embrittlement and raises the high-temperature strength of the core. In tube form the grade is used for components where a tough core and a hard, wear-resistant surface are both needed: drive shafts, camshafts, gear blanks, bushings, piston pins, drill string components and machined sleeves.
Chemical Composition and What Each Element Does
The composition below is the range generally applied to 20CrMo under the Chinese alloy structural steel standard, with the nearest equivalent Japanese grade shown for comparison. Values are percent by mass and are stated as heat analysis ranges.
| Element | 20CrMo range | JIS SCM420 reference | Effect on tube behaviour |
|---|---|---|---|
| Carbon | 0.17-0.24 | 0.18-0.23 | sets core strength and case carbon potential after carburising |
| Silicon | 0.17-0.37 | 0.15-0.35 | deoxidation; too high a level lowers forgeability |
| Manganese | 0.40-0.70 | 0.55-0.90 | hardenability and sulphur control |
| Chromium | 0.80-1.10 | 0.85-1.25 | hardenability, wear resistance, scaling resistance |
| Molybdenum | 0.15-0.25 | 0.15-0.30 | creep strength, resistance to temper embrittlement |
| Phosphorus | 0.025 max | 0.030 max | tramp element, restricted for toughness |
| Sulphur | 0.025 max | 0.030 max | machinability against transverse ductility |
| Copper | 0.30 max | 0.30 max | residual from scrap, restricted for hot ductility |
Two composition points deserve attention in a technical review. First, the carbon range is narrow but the consequences of drifting within it are not: a heat at 0.24 percent carbon behaves noticeably harder after quenching than a heat at 0.17 percent, and a fabricator who sets carburising parameters against one heat may find the next one different. Second, molybdenum is the element that separates 20CrMo from a plain 20Cr or 40Cr grade in high-temperature use, and a certificate showing molybdenum near the lower limit should be examined together with the tempering temperature, because both determine the creep resistance of the finished part.
Mechanical Properties in the Quenched and Tempered Condition
The properties below are the typical acceptance figures for 20CrMo in the quenched and tempered condition, with the corresponding hardness ceiling that applies before heat treatment or in the annealed delivery state. They are stated for reference specimens and are not a substitute for the values written on the order.
| Property | Typical requirement | Test basis |
|---|---|---|
| Tensile strength Rm | 885 MPa minimum | longitudinal specimen |
| Yield strength ReL or Rp0.2 | 685 MPa minimum | 0.2 percent proof for tube sections |
| Elongation A | 12 percent minimum | gauge length 5 diameters or 50 mm |
| Reduction of area Z | 50 percent minimum | tensile specimen fracture face |
| Impact energy KV2 | 78 J minimum | room temperature, Charpy V-notch |
| Hardness, annealed delivery | 197 HBW maximum | brinell, representative location |
The pairing of 885 MPa tensile with 685 MPa yield implies a yield-to-tensile ratio near 0.77, which is typical of a properly tempered low-alloy steel and leaves enough work-hardening capacity for cold forming. A ratio pushed above 0.85 by under-tempering is a warning sign: the part will machine badly, will be sensitive to hydrogen cracking after plating, and will lose toughness in service at low temperature.
Hardness is the property most often used for acceptance on tube, because it can be measured without destroying the component. The 197 HBW ceiling applies to the annealed or normalized delivery condition; after quenching and tempering, the acceptance value is normally agreed between purchaser and heat treater and checked at three locations per length, avoiding the decarburised skin.
Product Forms, Standards and Dimensional Control
20CrMo tube is supplied under a family of Chinese standards rather than a single one, and the correct standard depends on the application. Seamless steel tube for general structural and mechanical use is covered by GB/T 8162, which fixes the dimensional tolerances and the delivery condition but does not impose a fluid-service test regime. Seamless tube for fluid conveying is covered by GB/T 8163, which adds the hydrostatic test and the flattening and bending requirements. High-pressure boiler and superheater service uses GB/T 5310 with its own grade suffix system, and high-pressure chemical fertiliser equipment uses GB/T 6479. The alloy structural steel grade itself, including the chemistry ranges above, is defined in GB/T 3077.
Dimensional control follows the same pattern as for any cold-drawn or hot-rolled tube: outside diameter tolerance, wall thickness tolerance, eccentricity, straightness, and length tolerance. For machined components the wall thickness tolerance matters more than the outside diameter tolerance, because the machined bore is referenced to the outside surface and an eccentric wall forces a deeper cut on one side. A purchaser who needs a concentric wall should specify the eccentricity limit rather than accept the general tolerance, and should require the mill to measure it at both ends of each length.
Heat Treatment Routes: Carburising, Quenching and Tempering
20CrMo is normally delivered annealed or normalized, then heat treated by the component maker. Three routes dominate. Carburising followed by direct quenching and low-temperature tempering produces a case of 0.6 mm to 1.2 mm at 58 HRC to 62 HRC over a tough core, and is used for gears, cams and wear surfaces. Through-hardening by austenitising, oil quenching and tempering at 500 C to 650 C produces the 885 MPa class of properties listed above and is used for shafts and structural parts. Normalising is used when only machinability and dimensional stability are required.
Carburising atmosphere control is the step that decides whether the part meets its drawing. A carbon potential above the target produces retained austenite and a soft, unstable case; a carbon potential below target produces a case that is too shallow to support the design load and that will spall under contact fatigue. Case depth is verified on a sacrificial test piece or by hardness traverse on a sectioned part, and the acceptance rule is usually stated as the depth at which hardness falls to 550 HV.
Distortion is the practical limit on what can be achieved. Long thin-walled tube sections bend during oil quenching because the outside surface cools before the bore, and the resulting curvature may exceed the straightness tolerance. Press quenching, fixture quenching or a change to a lower-hardenability heat is the usual answer, and it must be settled before the tube is cut to length. Tempering after quenching is mandatory for this grade: an untempered martensitic structure in a 0.2 percent carbon steel is brittle and will crack at the first shock load.
Comparable Grades in Other Systems
Buyers comparing quotations from different regions need the equivalence map, but equivalence is never exact. The closest Japanese grade is JIS G4105 SCM420, which matches the carbon and molybdenum intent and sits slightly higher in chromium and manganese. The nearest American practice is a chromium-molybdenum carburising grade in the AISI 41xx family, but those grades carry different manganese and molybdenum balances and cannot be substituted without a fresh property review. European orders are usually written against EN 10216-2 or EN 10297-1 with a specific steel name, and the German designation system expresses the same idea as a carbon figure followed by chromium and molybdenum symbols.
Where an equivalent grade is proposed, three checks are enough to decide whether the substitution is safe: carbon and molybdenum must both be within the original intent, the hardenability must be demonstrated by a suitable test rather than assumed from chemistry, and the heat treatment must be re-qualified because a different hardenability shifts the quenching response. Substitution on chemistry alone is the most common cause of a part that passes the certificate review and fails in service.
Machining, Welding and Fabrication Notes
In the annealed condition 20CrMo machines reasonably well, but the molybdenum addition makes it stringier than a plain carbon steel and encourages built-up edge on high-speed tooling. Coated carbide inserts with a positive rake, generous coolant flow and a constant depth of cut give the best surface finish. Where the part will be carburised after machining, the machined surface finish should be better than that required at the end of the process, because the case replicates the underlying profile and a torn surface becomes a stress raiser under the hardened layer.
Welding is feasible but requires care. The grade is air-hardening at the section sizes used for tube, so a preheat in the region of 150 C to 250 C and a controlled cooling after welding are normally required, followed by a tempering treatment if the joint is to carry load. Filler metal should match the parent metal strength rather than the carbon content, and hydrogen-controlled consumables and a dry, clean joint face are essential, because 20CrMo is sensitive to hydrogen-assisted cracking in the heat-affected zone. Post-weld heat treatment, where applied, must stay below the tempering temperature used for the parent metal to avoid softening the tube body.
Cold forming is possible in the annealed state and the 12 percent minimum elongation gives adequate margin for moderate bending. After cold forming, a stress-relief anneal at a temperature below the tempering range restores dimensional stability, and it should be specified whenever the part is subsequently machined to a tight tolerance.
Inspection, Certificates and Acceptance Points
A 20CrMo tube order should carry four inspection deliverables. The first is a mill test certificate to EN 10204 type 3.1, issued by the steelmaker's own independent inspection, listing heat number, product analysis for each element in the specification, tensile results and the heat treatment condition. The second is a verification of the product analysis against the ranges in the table above, carried out by the purchaser on a sample if the application is critical. The third is a dimensional report covering outside diameter, wall thickness and eccentricity at both ends of each length. The fourth is the non-destructive test report where the application requires it: ultrasonic testing of the body wall, eddy current or magnetic particle testing of the surface, and a hydrostatic test where the fluid-service standard is invoked.
Traceability is the point that auditors examine most closely. The heat number on the certificate must match the heat number stencilled or stamped on the tube, and the transfer of that number through cutting, heat treatment and machining must be recorded. A tube that cannot be linked to its heat number is, for a pressure or safety-related application, unusable regardless of how good its properties are.
FAQ
Q: What does the 20 in 20CrMo mean?
The 20 records a nominal carbon content of about 0.20 percent, written in hundredths of a percent. The actual heat analysis range is typically 0.17 to 0.24 percent carbon. Chromium and molybdenum follow as element symbols because both are present at average levels below 1.5 percent, so no numeric multiplier is required after the symbol.
Q: Is 20CrMo the same as 40Cr?
No. 40Cr carries about 0.40 percent carbon with chromium and no deliberate molybdenum addition, and it is a quench-and-temper grade with higher attainable hardness and lower core toughness. 20CrMo has half the carbon, which is what makes it suitable for carburising, plus molybdenum for temper resistance. The two are not interchangeable in a heat-treated part.
Q: Why is molybdenum specified at only 0.15 to 0.25 percent?
Molybdenum is effective at low levels. At that range it raises hardenability, suppresses temper embrittlement during slow cooling after tempering, and improves creep resistance at elevated temperature. Adding more would raise cost without a proportionate property gain, and it would begin to affect weldability.
Q: Can 20CrMo tube be used without heat treatment?
It can be used in the annealed or normalized condition for lightly loaded machined parts, where the 197 HBW hardness ceiling and moderate strength are acceptable. Any part that relies on fatigue strength, wear resistance or a specified yield strength needs the quench and temper treatment, and the certificate should state the tempering temperature.
Q: What case depth is typical after carburising?
Most industrial components use a case of 0.6 mm to 1.2 mm measured to the 550 HV boundary, chosen against the contact stress and the allowable core strength. Deeper cases take many hours at temperature, grow the grain and increase distortion, so the depth should be set from the design load rather than from a general rule.
Q: Which certificate type should be requested for a pressure application?
An EN 10204 type 3.1 certificate issued by the steelmaker's independent inspection is the normal baseline, with the heat number traceable to the tube marking. Where a notified body or a purchaser's inspector is involved, a type 3.2 certificate or a witnessed test may be required instead.
Q: How should 20CrMo tube be stored before heat treatment?
Keep it dry and separated from carbon steel dust and grit, cap the ends and avoid stacking direct contact between lengths. Rust pits on the surface become stress raisers under a carburised case, so surface condition before heat treatment has a direct effect on fatigue life.