Nov 11, 2024 Leave a message

API Casing Steel Grades: J55, K55, N80, L80 and P110 Compared

What the API 5CT Grade Symbol Actually Controls

Any casing string is a stack of competing requirements: burst from internal pressure, collapse from external pressure, tensile load from the string's own weight plus overpull, and a service environment that may contain hydrogen sulfide, carbon dioxide or chlorides. The grade marked on the pipe is the mill's guarantee for one leg of that stack - the minimum yield strength of the pipe body - and it simultaneously fixes the chemistry, the heat treatment route and the test regime that the mill must apply to reach it. That is why two pipes with identical dimensions but different grade symbols behave completely differently in a well, and why the grade designation is the single most consequential line on a casing purchase order.

API SPEC 5CT is the specification that governs casing (and tubing, coupling stock and pup joints) for well service. It defines the grades in common use, the dimensional tables that go with them, the heat treatment conditions, the mechanical property ranges, the inspection and test requirements, and the marking rules that allow a joint to carry the API monogram. Around that core sit API SPEC 5B for thread dimensions and gauging, API RP 5C1 for care and running practice, and ISO 15156 / NACE MR0175 for service in sour environments. A purchaser who knows only the grade name and not the rest of that envelope is buying a strength class without a service capability.

The five grades that dominate real orders - H40, J55, K55, N80, L80 and P110, with C90, T95 and Q125 appearing on the more demanding strings - are not a simple ladder from weak to strong. Between L80 and N80 the ladder actually crosses: L80 is deliberately capped at a narrower and lower yield window than the top of the N80 window, because L80 is a sour-service grade where hardness control outranks strength. Understanding that inversion is the first step in reading the grade system correctly.

The Grade Family and How the Designations Are Built

Most grade symbols follow one pattern: a letter followed by a number, where the number is the nominal minimum yield strength in thousands of pounds per square inch. J55 therefore means a nominal 55 000 psi minimum yield, P110 means 110 000 psi, and Q125 means 125 000 psi. The leading letter does not encode a chemistry; it is simply a designation that carries the grade's individual combination of chemistry limits, heat treatment and test requirements.

H40 is the lowest grade in routine oilfield use, a plain-carbon pipe intended for shallow, low-pressure service such as surface strings, conductor pipe and water-disposal wells. It is normally supplied as-rolled with no heat treatment obligation, and its wide yield band gives the mill latitude that the higher grades do not have.

J55 is the workhorse of shallow and medium-depth oil wells. It is a plain-carbon, as-rolled grade with useful ductility and a tensile minimum of 517 MPa, which is high relative to its yield minimum - the grade is forgiving in handling and threading, which is much of its commercial value.

K55 sits alongside J55 with an identical yield window but a higher tensile minimum of 655 MPa. The practical difference in the field is not corrosion resistance; it is toughness and load capacity headroom. K55 is often chosen for service where casing must also tolerate handling abuse or where a transition string must carry more tensile load than J55 comfortably allows.

N80 exists in two delivery conditions that are frequently confused. N80-1 is supplied in the normalized condition, with a ferritic-pearlitic microstructure produced by normalizing or by controlled rolling. N80-Q is quenched and tempered, giving a tempered martensitic structure, higher and more uniform toughness, and better resistance to brittle behaviour at low temperature. Both deliver the same 552 to 758 MPa yield window and 689 MPa tensile minimum, but they are not interchangeable for low-temperature or impact-critical service, and the purchase order must state which type is required.

L80 is the standard sour-service grade. Three types are defined: L80-1 for the conventional low-alloy chemistry, L80-9Cr with roughly 9 % chromium, and L80-13Cr with 12 to 14 % chromium. All three are quenched and tempered and all three are subject to a maximum hardness of 23 HRC, which is the property that makes them usable in wet hydrogen sulfide service. None of the L80 types may be supplied as welded pipe.

C90 and T95 are the intermediate sour-service grades, offering 621 to 724 MPa and 655 to 758 MPa yield respectively. Each is defined with two numbered types that allow different chemistry and heat treatment routes to reach the same strength band while keeping hardness below 25.5 HRC. They exist because a well can be both sour and deep, where L80 collapse resistance is insufficient but P110 is not permitted by the sour-service standards.

P110 is the high-strength grade that carries most deep and high-pressure completions. It is quenched and tempered, its yield window runs from 758 to 965 MPa, and it is normally specified with a minimum tensile of 862 MPa. The letter P here is part of the grade symbol and not a delivery-condition suffix; the same is true of the T in T95. Suffixes that do carry meaning are the Q of N80-Q, the numeric types of C90 and T95, and the chromium designations of L80.

Q125 extends the ladder to 862 to 1034 MPa yield with a 931 MPa tensile minimum, and it is defined with several numbered types that distinguish alloy designs delivering the same strength. Q125 is a specialist grade for ultra-deep, very high-pressure strings, and it demands correspondingly careful design because toughness margin and sour-service tolerance both shrink as strength rises.

Yield and Tensile Strength Windows by Grade

The table below summarises the pipe-body requirements that drive string design. Yield strength is the 0.5 % extension under load value measured in accordance with the specification; tensile strength is the ultimate value from the same longitudinal specimen. Where a maximum is not stated by the grade, the mill is free to exceed the minimum, which is precisely why a purchaser checking a mill test certificate should read both ends of the window rather than only the minimum.

Grade / type Yield strength, MPa Tensile strength, MPa Hardness ceiling Delivery condition
H40 276 to 552 414 minimum Not specified As-rolled
J55 379 to 552 517 minimum Not specified As-rolled
K55 379 to 552 655 minimum Not specified As-rolled
M65 448 to 586 586 minimum 22 HRC maximum As-rolled or normalized
N80-1 552 to 758 689 minimum Not specified Normalized or controlled rolled
N80-Q 552 to 758 689 minimum Not specified Quenched and tempered
L80-1 / L80-9Cr / L80-13Cr 552 to 655 655 minimum 23 HRC maximum Quenched and tempered
C90-1 / C90-2 621 to 724 689 minimum 25.5 HRC maximum Quenched and tempered
T95-1 / T95-2 655 to 758 724 minimum 25.5 HRC maximum Quenched and tempered
P110 758 to 965 862 minimum Controlled by grade practice Quenched and tempered
Q125 862 to 1034 931 minimum Controlled by grade practice Quenched and tempered

The ratio between tensile minimum and yield minimum is itself informative. For J55 the ratio is about 1.36, for K55 about 1.73, and for N80 about 1.25; for the sour-service grades the tensile minimum sits closer to the yield maximum, which means the window is narrow and the mill has very little room to work with. A narrow window is harder to produce and is one of the reasons L80 and T95 carry a price premium over a J55 of the same dimensions.

Note also that the tightest window in the table belongs to L80: 552 to 655 MPa yield with a 655 MPa tensile minimum. Any heat treatment drift that pushes hardness up will breach the 23 HRC ceiling, and any drift downwards will breach the yield minimum. This is why L80 pipe is normally supplied with a full hardness survey rather than a single check.

Chemistry and Heat Treatment Logic Behind Each Grade

For the plain-carbon grades H40, J55 and K55 the specification fixes the mechanical result and leaves the steelmaker to select a carbon-manganese composition that reaches it, subject to ceilings on phosphorus and sulfur. In practice these grades are medium-carbon steels rolled to finished size and cooled in air; no heat treatment is obligatory, and the produced properties come from composition plus finishing temperature. That is what keeps them inexpensive, and it is also why their property scatter is wider than that of a quenched and tempered grade.

From L80 upward the chemistry becomes part of the guarantee. The tables impose element-by-element limits on carbon, manganese, chromium, molybdenum, nickel, phosphorus and sulfur because two things must be protected at once: hardenability, so that the section quenches through to a martensitic structure, and the hardness ceiling, which cannot be met if carbon or residual elements run high. Sulfur control matters twice over in the sour grades, since manganese sulfide inclusions are initiation sites for sulfide stress cracking and for hydrogen-induced cracking.

The chromium-bearing L80 types add a corrosion-resistance argument to the strength argument. L80-9Cr and L80-13Cr are martensitic stainless steels; the 12 to 14 % chromium of the 13Cr type provides a passive film that resists carbon dioxide corrosion, while the carbon content is held in a narrow band so that the as-quenched structure can be tempered back below 23 HRC without losing the strength the grade requires. Neither may be welded, and both demand a genuine quenching line rather than an in-line normalizing pass. A mill that offers L80-13Cr without a dedicated austenitizing, quenching and tempering route cannot be making the real product.

For N80 there is a practical warning. Because the type 1 and type Q variants share a name, purchase orders that simply state N80 will be filled with whichever type the mill prefers. Where impact toughness at low temperature matters, or where the string will see dynamic loads, state N80-Q explicitly and require the corresponding impact test results on the certificate.

Depth and Pressure Layering: Matching Grade to Well

Field practice groups grades by depth and pressure band, but the bands are a starting point rather than a design rule. A shallow vertical well with modest surface pressure is routinely completed in J55 or K55, where burst and collapse loads are low, the string is short, and the cost of a higher grade buys nothing. H40 appears mainly in conductor and surface pipe, and in water or disposal service where pressures are trivial.

Medium-depth wells, roughly 2 000 to 3 500 m in typical land service, are the natural territory of N80. The grade provides enough burst and collapse capacity for moderate pressure, tolerates the tensile load of a longer string, and remains ductile enough for routine handling. Most of the world's production casing in this band is N80-1 or N80-Q depending on the toughness requirement.

Deep wells, in the 3 500 to 5 000 m range, force a choice between L80 and P110. Where the environment is sweet and the loads are high, P110 is the straightforward answer. Where hydrogen sulfide is present, the choice collapses to L80, C90 or T95, and the design must then be reworked around their more limited collapse and burst capacity rather than around the loads that P110 would have carried. This is the point where grade selection becomes a wall-thickness and connection problem, not just a steel problem.

Beyond about 5 000 m, and in high-pressure high-temperature gas wells, P110 and Q125 come into play, often with heavy wall and premium connections. At this level the design must be triaxial: the interaction of burst, collapse and tension, plus the effect of elevated temperature on yield strength. The specification includes elevated-temperature yield data for the common grades, and a string designed on room-temperature yield at 150 °C bottomhole temperature is over-designed in the wrong direction, since yield falls as temperature rises.

Grade escalation is the crudest available lever. Increasing wall thickness, changing the connection, or re-tapering the string frequently delivers the required capacity at lower cost and with better toughness than jumping a grade. A string that needs 15 % more burst capacity is usually better served by one wall step than by a grade step, because the grade step also removes sour-service tolerance that may be needed later in the well's life.

Sour Service: The Hard Ceiling on High-Strength Grades

Wet hydrogen sulfide changes the rules completely. In the presence of H2S and free water, atomic hydrogen can enter the steel and embrittle it, producing sulfide stress cracking at stress levels far below the yield strength. The failure is brittle and sudden, which is why the industry treats it as a design constraint rather than a corrosion allowance. ISO 15156 and NACE MR0175 set the qualification framework, and the trigger for sour service is normally a hydrogen sulfide partial pressure at or above about 0.3 kPa in the gas phase, together with the presence of free water.

The controlling variable for carbon and low-alloy steels is hardness. Above roughly 22 HRC the susceptibility of these steels to sulfide stress cracking rises steeply, and that single number explains why P110 and Q125 are excluded from sour service regardless of how much collapse capacity a designer would like. P110 is quenched and tempered to a hardness level that sits well above the ceiling, and no amount of supplementary testing converts it into a sour-service grade for general use. Any proposal to run P110 in a sour well should be treated as a design error unless a specific, documented qualification programme covering the exact chemistry, hardness distribution and environment has been completed.

L80 is the grade that fits under the hardness ceiling by construction. Its 23 HRC maximum, combined with low sulfur and a tempered martensitic structure, gives it the toughness to resist cracking in moderate H2S partial pressures. Where the well is deeper, C90 and T95 provide more strength while remaining inside the 25.5 HRC ceiling that the standards accept for these grades, and their two numbered types exist precisely to let mills reach that strength band through different alloy and heat treatment combinations.

Qualification testing is not optional in this space. Sulfide stress cracking resistance is demonstrated by tensile testing in an acidified, H2S-saturated brine in accordance with NACE TM0177, and where the service is also wet and contains H2S, resistance to hydrogen-induced cracking is demonstrated by the immersion test of NACE TM0284. Certificates for sour-service casing should carry these results by heat number, alongside the hardness survey, not as a generic statement of compliance.

There is a second sour-service trap: temperature. Susceptibility to sulfide stress cracking generally decreases as temperature rises, which is why some deep, hot wells can be completed in a grade that would be unacceptable at the surface. The evaluation must be done at the temperature of the section concerned, and the surface wellhead area must be evaluated at surface temperature even when the bottomhole condition looks benign.

Carbon Dioxide and Chloride Service: Where 13Cr Belongs

Sweet corrosion driven by carbon dioxide in the presence of water is a different mechanism, and it is managed differently. Carbon steel corrodes at a rate set by the CO2 partial pressure, temperature, flow regime and water chemistry, and the usual answers are inhibition, coating, or a corrosion-resistant alloy. L80-13Cr belongs to the third answer: the 12 to 14 % chromium content forms a chromium oxide film that is stable in CO2 environments and reduces general corrosion by an order of magnitude or more compared with carbon steel.

The boundary of 13Cr is set by temperature and by chlorides. As temperature rises above roughly 150 °C the passive film becomes less protective in CO2 service, and general corrosion rates climb; at the same time, high chloride content in the produced water raises the risk of pitting and of chloride stress corrosion cracking. The grade is therefore applied in a window that is hot enough for CO2 corrosion to be a problem but not so hot that the film breaks down, and with chloride levels that the operator's corrosion study shows to be tolerable.

Hydrogen sulfide is the hard limit for martensitic 13Cr. These steels tolerate only very small H2S partial pressures, measured in fractions of a kilopascal in most published service envelopes, before sulfide stress cracking becomes a risk. A well that starts sweet and turns sour will take a 13Cr completion outside its envelope, which is why the decision to use it should be based on a full compositional forecast over field life rather than on the initial production analysis.

Where higher strength is needed in a CO2 environment, modified martensitic stainless grades in the 95 ksi and 110 ksi classes exist, with tightened chemistry and stricter heat treatment. They are not standard API grades and must be qualified against the specific environment. L80-9Cr sits between carbon steel and 13Cr: useful where a moderate improvement in CO2 resistance justifies the alloy premium, but not a substitute for 13Cr in aggressive water.

Threads and Connections under API SPEC 5B

Three API thread forms cover the great majority of casing: short round thread, long round thread and buttress. All three are defined dimensionally and by gauging practice in API SPEC 5B, and the choice between them is driven by wall thickness, diameter, pressure and whether the well produces gas.

Short round thread casing is the low-cost standard, with eight threads per inch and a relatively short engaged length. It suits small to medium diameters and moderate pressures, and it is the natural pairing for J55 and K55 strings in shallower wells. Long round thread casing uses the same eight-thread-per-inch form but a longer thread and coupling, giving more engaged length and higher joint strength; it is the usual choice where tensile load or pressure approaches the limit of the short form.

Buttress thread casing uses a five-thread-per-inch form with a load-bearing flank that is close to perpendicular to the axis. That geometry gives much higher joint strength in the heavy walls and large diameters used for deep strings, which is why buttress is standard on 9-5/8 in and larger intermediate casing and on heavy-wall production strings. Buttress is not a gas-tight seal in the way a premium connection is; it relies on thread compound and interference for sealing.

Premium connections, with metal-to-metal seals and shouldering torque surfaces, are specified where gas tightness under cycling pressure is required, where clearance is limited, or where the casing must be rotated or drilled. They are proprietary products, so the connection data must come from the connection supplier rather than from the pipe specification, and the pipe body must be ordered with dimensions that match the connection's requirements.

Running practice matters as much as the thread form. Make-up torque must follow the connection supplier's value, thread compound must be applied to the full engaged length, and the pipe must be aligned before stabbing. API RP 5C1 covers handling, running and care of casing, and most connection failures in the field trace back to a departure from it rather than to a defective thread.

Wall Thickness, Unit Weight and Dimensional Control

Unit weight is the purchaser's shorthand for wall thickness, and the two must be read together. The table below lists common casing sizes with the wall thickness that corresponds to each weight; the same outside diameter at a different weight is a different pressure vessel, and a grade change will not compensate for a wall change.

Outside diameter Unit weight Wall thickness, mm Typical API thread form
4-1/2 in (114.3 mm) 11.60 lb/ft 6.88 Short or long round thread
5-1/2 in (139.7 mm) 17.00 lb/ft 7.72 Short or long round thread
5-1/2 in (139.7 mm) 23.00 lb/ft 10.54 Buttress
7 in (177.8 mm) 26.00 lb/ft 9.19 Long round thread or buttress
9-5/8 in (244.5 mm) 47.00 lb/ft 10.03 Buttress
13-3/8 in (339.7 mm) 68.00 lb/ft 10.92 Buttress

Dimensional acceptance is not limited to wall thickness. Outside diameter tolerance, out-of-roundness, straightness, drift diameter and length range all appear in the specification, and each is checked at the mill and can be checked again on receipt. Wall thickness is normally permitted to run under the nominal value by a stated percentage, with no plus tolerance beyond the weight allowance, so a joint can be at nominal weight and still have a wall below nominal at any given point. That is why wall thickness is verified by ultrasonic scanning along the body rather than by weighing the joint.

Length range is a frequent source of confusion in shipping documents. Casing is supplied in three ranges, roughly 4.88 to 7.62 m, 7.62 to 10.36 m and 10.36 to 14.63 m, and the range must be stated on the order because it determines how the string is tallied and how the pipe is stacked and transported. Mixing ranges in a single string complicates handling and is normally avoided.

Drift testing confirms that the bore is clear enough for the tools that will pass through it. The drift mandrel diameter is tabulated by size and weight, and the test is a go/no-go check that must be recorded on the inspection documents. A joint that passes hydrostatic testing but fails drift is not acceptable casing.

Manufacturing Route, Inspection and Certification

Casing is made predominantly by the seamless route: a billet is pierced and elongated on a mandrel mill, plug mill or premium quality finishing mill, then sized and straightened. For the quenched and tempered grades the pipe passes through a dedicated austenitizing furnace, a quench and a tempering furnace, with the tempering temperature set to land the yield inside the grade window while keeping hardness under the ceiling. Welded casing exists for the lower grades, typically electric resistance welded from coil, but the higher grades, all sour-service grades and all chromium-bearing grades are seamless only.

Hydrostatic testing is the primary pressure proof. The test pressure is calculated from the thin-wall formula relating pressure to wall thickness, outside diameter and a specified fibre stress, and the specification tabulates standard test pressures by size, weight and grade while capping them at a practical maximum. Holding time must be at the specified pressure for the specified duration with no leakage, and the record must identify the joint.

Non-destructive examination covers the pipe body and, where specified, the end areas. Electromagnetic inspection is used for longitudinal and transverse defects in the body, ultrasonic inspection for wall thickness and laminar defects, and magnetic particle or liquid penetrant inspection for the threads and the coupling after machining. Flux leakage inspection of the seamless body is standard practice on the higher grades.

Mechanical testing is destructive and sample-based: tensile tests to verify yield and tensile strength, flattening or hardness tests as the grade requires, and Charpy V-notch impact tests for the grades that carry an absorbed energy requirement. The sour-service grades L80, C90 and T95 are impact tested as a matter of routine, and supplementary low-temperature impact requirements can be ordered for the other grades where the well is cold.

Documentation is where a purchase is either confirmed or lost. A mill test certificate issued to EN 10204 3.1, traceable to heat number and to the specific joints, should carry chemistry, heat treatment records, tensile results, hardness survey, impact results, hydrostatic test pressure and duration, non-destructive examination method and result, and dimensional verification. Where the pipe carries the API monogram, the mill holds a licence and the marking on each joint must correspond to the certificate. Third-party inspection at the mill, covering witnessing of the hydrostatic test and review of the records, is common on sour-service and high-pressure orders.

Grade Selection Logic and the Mistakes That Cost Strings

A defensible selection sequence runs as follows. Establish the load cases for burst, collapse and tension from the well design, including the worn and the evacuated cases. Establish the environment: hydrogen sulfide partial pressure, carbon dioxide partial pressure, chloride content, temperature profile and pH, by section. Screen the candidate grades against the environment first, which will eliminate P110 and Q125 immediately if the well is sour. Then, within the surviving grades, select wall thickness and diameter to satisfy the load cases with the design factors required. Finally, select the connection against the pressure, gas tightness and handling requirements, and verify that the pipe body dimensions ordered match the connection.

The most expensive error in the field is running P110 in a well with hydrogen sulfide. It happens because the grade is the familiar high-strength choice, because the load cases were calculated before the gas analysis came back, or because a supplier offered it as equivalent. The consequence is a string operating outside the qualification of its own material, with brittle failure as the failure mode.

A second common error is assuming that K55 is more corrosion resistant than J55. Both are plain-carbon, as-rolled grades with no alloy addition for corrosion resistance; the difference between them is tensile strength, not corrosion behaviour. Where corrosion is the issue, the answer is a chromium-bearing grade or a different mitigation, not a neighbouring carbon grade.

A third is treating L80 as a stronger grade than N80 because of the letter ordering. L80 is capped at 655 MPa maximum yield, below the top of the N80 window, and it is chosen for hardness control in sour service rather than for strength. Designers who substitute L80 for N80 expecting more capacity will find less.

A fourth is buying N80 without stating the type. N80-1 and N80-Q arrive with different microstructures and different toughness, and a certificate showing N80 alone does not tell the buyer which one was supplied.

A fifth is upgrading grade where wall thickness was the real deficiency. Collapse resistance depends strongly on the diameter-to-wall ratio, and a thin-wall P110 can have lower collapse resistance than a heavier-wall J55 of the same diameter. Grade and geometry must be optimised together.

A sixth is applying 13Cr to any well with CO2 without checking temperature and chlorides, or carrying a 13Cr completion into a field that turns sour later in life. A seventh is specifying buttress thread on small-diameter, thin-wall pipe where the wall cannot support the thread depth, when round thread is the correct and cheaper answer. An eighth is neglecting handling: high-strength quenched and tempered pipe is more sensitive to elevator marks, tong bites and impact damage than as-rolled J55, and a deep scratch on a P110 joint is a stress concentration in a material with limited plastic reserve.

Finally, storage and transport deserve a line of their own. Threads must be protected with the specified protectors, couplings must not be used as lifting points, pipe must be stacked on dunnage clear of the ground, and chromium-bearing grades should be kept away from carbon steel contact to avoid galvanic staining. Damage found at the rack is cheap to fix; the same damage found at 4 000 m is not.

FAQ

Q: Which API casing grades are used most often, and why?
J55, K55, N80, L80 and P110 account for the great majority of casing orders. J55 and K55 cover shallow and medium wells at low cost, N80 covers medium-depth and moderate-pressure service, L80 covers sour service within the 23 HRC hardness ceiling, and P110 covers deep, high-pressure sweet wells with a 758 to 965 MPa yield window.

Q: What is the difference between N80-1 and N80-Q?
Both deliver 552 to 758 MPa yield and a 689 MPa tensile minimum. N80-1 is supplied normalized or controlled rolled with a ferritic-pearlitic structure, while N80-Q is quenched and tempered with a tempered martensitic structure that gives better and more uniform toughness, so the type should always be stated on the purchase order.

Q: Can P110 casing be used in a well containing hydrogen sulfide?
No, not in general service. The hardness level of P110 sits well above the roughly 22 HRC ceiling that ISO 15156 and NACE MR0175 apply to carbon and low-alloy steels for resistance to sulfide stress cracking. Sour wells are completed in L80, C90 or T95, with strength made up through wall thickness and connection design instead of grade.

Q: Why is L80's maximum yield lower than N80's maximum yield?
Because L80 is a sour-service grade defined by hardness control rather than by maximum strength. Its window of 552 to 655 MPa yield with a 655 MPa tensile minimum, combined with a 23 HRC maximum hardness, keeps the steel below the hardness level at which sulfide stress cracking becomes likely, which is a more valuable property in a sour well than the extra 100 MPa of yield that N80 can reach.

Q: When should 13Cr casing be chosen over carbon steel?
When carbon dioxide partial pressure and temperature are high enough that inhibited carbon steel cannot hold corrosion within the design allowance, and when chlorides and hydrogen sulfide are low enough to stay inside the martensitic stainless envelope. Temperatures above roughly 150 °C and more than trace hydrogen sulfide content usually take 13Cr out of consideration.

Q: What do short round, long round and buttress threads correspond to in API SPEC 5B?
Short round thread and long round thread use an eight-thread-per-inch form, with the long version giving more engaged length and higher joint strength. Buttress uses a five-thread-per-inch form with a near-vertical load flank, which provides much higher joint strength for heavy-wall and large-diameter deep strings.

Q: Which documents should accompany a casing shipment?
A mill test certificate to EN 10204 3.1 traceable to heat number, showing chemistry, heat treatment condition, tensile and yield results, hardness survey where applicable, impact results for the grades that require them, hydrostatic test pressure and duration, non-destructive examination records, dimensional and drift verification, plus the API monogram marking correspondence where the pipe is licensed.

Send Inquiry