What Double Submerged Arc Welding Means for a Straight Seam Pipe
Double submerged arc welded pipe, usually abbreviated DSAW, describes a longitudinally seamed pipe in which the straight seam is welded from the inside and from the outside by submerged arc welding. In the designation system of API SPEC 5L the product appears as pipe type SAWL, and in Chinese and European procurement documents it is commonly called LSAW pipe. The word double refers only to the two-sided welding of a single seam; it does not mean two seams, and it does not by itself imply a higher grade. What it does imply is full-thickness fusion and a weld whose metal and heat-affected zone must be separately qualified for strength, hardness and toughness.
The process exists because a single-sided weld cannot reliably fuse the full wall of a heavy plate without either a very wide, high-heat-input bead that damages toughness or a backing system that is impractical at production rates. Welding one side, rotating or indexing the shell, and welding the second side allows a controlled, symmetrical heat input, a sound root on the inside, and a finished seam whose cap can be ground flush where internal flow or pigging demands it.
Step One: Plate Selection and Preparation
DSAW starts from discrete plate, not coil. The plate specification is normally a pipeline plate grade matched to the finished pipe grade, ordered with a controlled carbon equivalent, a restricted sulphur level for inclusion shape control and, for low-temperature service, a guaranteed Charpy energy in the plate transverse direction. Plate is usually accepted with ultrasonic examination to ASTM A578 to exclude laminations near the seam preparation, because a lamination within the weld preparation becomes a crack-like planar defect that no amount of welding can repair.
Edge preparation is the first real production step: the plate is cut to width with a tolerance that directly determines the finished circumference, then the two long edges are milled or planed to a bevel. The bevel geometry is designed so that the inside pass and the outside pass each have adequate access, typically an X-type or double-V preparation with a root face of a few millimetres. Edge straightness matters as much as the bevel angle, because a wavy edge cannot be closed to a uniform root gap and will produce variable penetration along the seam. After milling, edges are cleaned of oil, mill scale, rust and moisture; residual hydrocarbons in the bevel are a direct source of porosity and diffusible hydrogen.
Plates are also pre-bent at the edges in a crimping press so that the finished pipe does not develop a flat spot at the seam. This crimping step is easy to overlook when auditing a mill, yet it is the difference between a round pipe and one that needs excessive force to close during girth welding.
Step Two: Forming the Shell
Three forming routes dominate. The UOE route presses the plate first into a U shape, then into an O shape, and closes the seam with an O-ing press; the pipe is subsequently expanded mechanically or hydraulically. The JCOE route forms the plate incrementally, one step at a time, first into a J profile and then into a C profile, using a large press with a stepped die; the edges are pre-bent, then the shell is closed and the seam is tack welded before expansion. The three-roll bending route rolls the plate between rolls until the circumference closes, and it is common for smaller diameters and for short runs.
Whichever route is used, the forming operation sets the two properties that later determine roundness and weldability: the gap and misalignment at the seam, and the residual stress locked into the shell. Seam misalignment is measured as the offset between the plate edges on the outside and inside surfaces and is normally limited to a fraction of the wall thickness by the purchase specification, not only by the mill's internal standard. Edge misalignment that exceeds the limit creates a stress concentration at the weld toe and a step that the ultrasonic probe cannot easily interpret.
Step Three: Tack Welding and the Two Weld Passes
After closing, the seam is tack welded, usually by submerged arc or by gas metal arc welding, with tacks spaced along the seam and of sufficient length to hold the shell during handling. The shell is then transferred to the internal welding station, where a submerged arc head positioned on a boom inside the pipe deposits the internal pass. Flux is fed ahead of the arc and recovered by a suction system behind it; the arc is completely covered, which is the defining feature of the process and the reason it produces a clean weld with little spatter and no visible arc light.
The pipe is then transferred to the external welding station, where the outside pass is deposited over the same seam. The two passes must be sequenced and dimensioned so that the second pass refines and tempers part of the first, achieving full penetration through the wall with a controlled overlap. In some plants the two passes are made simultaneously with a single pair of heads on opposite sides; this reduces distortion and heat input per side, but it demands precise alignment of the root gap and much tighter process control, so it is normally reserved for high-volume production of a stable size.
Critical variables at this stage are welding current, arc voltage, travel speed, wire diameter and number of wires, flux type and flux condition, preheat and interpass temperature. Flux must be baked before use to drive off moisture, and recycled flux must be screened and blended within limits, because damp or contaminated flux is the most common cause of hydrogen-induced cracking in the seam. Heavy wall pipe is preheated, and the interpass temperature is capped to protect the toughness of the heat-affected zone.
Process Stages and Control Points
| Stage | Key operation | Control point to verify |
|---|---|---|
| Plate receipt | Ultrasonic examination, grade verification | No laminations near edges; heat number traceable to the pipe |
| Edge preparation | Cutting, milling or planing of bevels | Bevel angle, root face, edge straightness, width tolerance |
| Pre-bending | Crimping of plate edges | Edge curvature matches the finished radius |
| Forming | UOE, JCOE or three-roll bending | Seam gap, radial misalignment, circumference |
| Tack welding | Temporary seam closure | Tack length and spacing, absence of cracks |
| Internal welding | Submerged arc pass on the inside seam | Current, voltage, speed, flux condition, preheat |
| External welding | Submerged arc pass on the outside seam | Penetration, cap width, overlap with the internal pass |
| Seam grinding | Cap and toe finishing | Flush cap where specified, no grinding gouges, smooth toe |
| Expansion | Cold mechanical or hydraulic expansion | Expansion ratio, ovality, diameter after expansion |
| Non-destructive testing | Ultrasonic and radiographic seam inspection | Coverage of full seam length at both ends |
| Hydrostatic test | Pressure test to specified hoop stress | Hold time, pressure record, no leakage or sweating |
| End finishing | Beveling, facing, end squareness | Bevel angle, root face, internal diameter at ends |
| Coating and marking | External coating, stencil, bundle tagging | Coating thickness and continuity, heat and pipe number |
Why Two-Sided Welding Changes the Mechanical Result
The engineering argument for the double pass is not cosmetic. Welding from both sides delivers full penetration, so the joint is not dependent on a narrow root bead for its integrity; the toe of each pass is on the surface where it can be inspected and ground; and the heat input is shared, which reduces the peak temperature seen by any one part of the heat-affected zone. The practical results are a weld with a more uniform hardness profile, a lower risk of incomplete fusion at mid-wall, and a joint that responds predictably to girth welding in the field.
Symmetry also helps distortion control. A single-sided heavy weld pulls the shell into a banana shape and closes the seam gap unevenly along the length; when the second pass is applied to a seam that has already been constrained by the first, the bending moment partly cancels. This is one reason DSAW pipe holds a rounder cross-section over its length than a single-pass longitudinal weld would allow, and it is also why the expansion step that follows is more effective.
The expansion step itself is a deliberate plastic deformation of roughly one percent of the circumference. It improves roundness and diameter tolerance, reduces the residual stress from welding and forming, and slightly raises the yield strength through work hardening while lowering the yield-to-tensile ratio spread. For strain-based design pipeline projects, the yield-to-tensile ratio and the uniform elongation after expansion are specified properties, not incidental outcomes, so the expansion ratio has to be controlled rather than maximised.
Inspection, Testing and Documentation
Seam inspection is performed on the full length of both the internal and external weld. Automated ultrasonic testing to ISO 10893-11, practiced in accordance with ASTM E213, detects planar lack of fusion and crack-like indications; radiographic testing to ISO 10893-6 or ASTM E94 detects slag, porosity and incomplete penetration in a sample or full length depending on the specification. Weld ends receive additional magnetic particle testing to ASTM E709 after beveling, because the beveling operation can open indications at the seam ends, and this is exactly where field girth welds will later be made.
Mechanical testing follows the qualified welding procedure and the purchase specification: transverse tensile tests across the seam, all-weld-metal tensile tests where required, guided bend tests with the weld in tension and in root tension, Charpy V-notch sets from the weld metal and the fusion line at the specified temperature, hardness traverses across the weld and heat-affected zone, and macroscopic examination of a seam section. For sour service, the hardness limit of 250 HV10 applies to the weld and the heat-affected zone, and the seam must pass the hydrogen-induced cracking evaluation required by ISO 15156 / NACE MR0175.
Each pipe carries a heat number, a pipe number and the mill's identification; the inspection certificate to EN 10204 type 3.1 must tie the delivered pipe to those numbers and to the actual test results. Coating records, weld procedure qualification records to ISO 15614-1, welder and operator qualification to ISO 9606-1 and ISO 14732, and the non-destructive testing procedure approvals complete the documentation package. Where the pipe is coated with fusion bonded epoxy to ISO 21809-2 or with three-layer polyethylene to DIN 30670, the coating certificate and the holiday test record belong in the same package.
Where DSAW Pipe Is the Correct Choice
DSAW is the natural choice for large-diameter, heavy-wall line pipe: high-pressure gas and oil transmission mains, compressor and pump station piping, offshore export lines and risers, and large structural tubulars. It is also used for water transmission and for penstock applications where the diameter exceeds what ERW can form. The size range typically starts around 406 mm outside diameter and extends to 1626 mm and beyond, with wall thickness from about 6 mm to 40 mm and heavier for special orders, in grades from Gr.B through X80 and in PSL1 or PSL2 quality levels as required by API SPEC 5L, ISO 3183 or GB/T 9711.
Where the diameter is small, the wall is thin and the pressure duty is moderate, ERW is the more economical answer, and where the diameter is extremely large relative to the available plate width, helical seam pipe allows a wide diameter to be produced from narrow strip. The decision should be driven by the design pressure, the design factor, the required toughness at the lowest expected operating temperature, the available inspection methods and the total installed cost, not by the nominal pipe type alone.
Frequently Observed Process Problems
Most DSAW rejections trace back to a small number of causes. Moisture in the flux or on the plate edges produces porosity and raises diffusible hydrogen; the remedy is flux baking and edge drying, not more grinding. Excessive heat input raises heat-affected zone hardness and lowers toughness, and it shows up as a failed Charpy set long after the pipe has been welded. Poor edge alignment produces a step at the seam that ultrasonic testing reports as a defect even when the weld is sound. Finally, skipping the crimping step or forming with worn rolls leaves a flat section that hydrostatic testing will not reveal but that will cause fit-up problems at the girth weld.
FAQ
Q: Is DSAW the same as LSAW?
In practice yes. DSAW describes the welding method, a straight longitudinal seam welded on both the inside and the outside by submerged arc welding. LSAW describes the seam orientation, longitudinal submerged arc welded, and this is the pipe type designation SAWL used in API SPEC 5L. A DSAW pipe is therefore an LSAW pipe, and the terms are used interchangeably in purchase documents.
Q: What plate and pipe standards apply to DSAW line pipe?
The finished pipe is normally specified to API SPEC 5L, ISO 3183 or GB/T 9711 in grades from Gr.B to X80, in PSL1 or PSL2 quality, with pipe type SAWL. Plate is ordered to a matching pipeline plate specification with controlled carbon equivalent and, for PSL2, guaranteed toughness. Dimensions follow ASME B36.10M for the nominal size and wall series, weld end preparation commonly follows ASME B16.25, and mechanical testing methods follow ASTM A370.
Q: Why must the flux be baked before submerged arc welding?
Submerged arc fluxes are hygroscopic. Absorbed moisture dissociates in the arc and supplies hydrogen to the weld pool, which can cause delayed cracking in the seam and in the heat-affected zone, particularly in heavy wall and in high-strength grades. Baking drives off the moisture, and the flux handling procedure, together with the recycle ratio and screening, is a legitimate audit item for any buyer of DSAW pipe for wet or sour service.
Q: How much expansion is applied after welding, and why?
Cold expansion of the order of one percent of the circumference is typical. It corrects ovality and diameter, relieves a large part of the welding and forming residual stress, and improves the roundness of the pipe ends so that field girth welding fit-up is predictable. Expansion also slightly raises yield strength and changes the yield-to-tensile ratio, so the expansion ratio is recorded and reported rather than treated as an informal mill habit.
Q: Can a DSAW seam be repaired?
Repair is permitted only within the limits of the purchase specification and the qualified repair procedure, and it normally requires removal of the defect by grinding to sound metal, confirmation by the applicable non-destructive method, and rewelding with a qualified procedure followed by re-inspection of the repaired area. Repairs are recorded against the pipe number. Cracks in the weld or heat-affected zone are generally not repairable by welding and cause rejection of the pipe.
Q: Which tests prove that a DSAW pipe meets PSL2 requirements?
A PSL2 pipe requires, in addition to the PSL1 requirements, specified impact testing of the pipe body, the weld seam and the heat-affected zone at a stated temperature, tighter chemical composition limits, and non-destructive inspection of the weld seam. The evidence in the certificate is the Charpy result set with its test temperature and shear appearance, the tensile results including the yield-to-tensile ratio, the hardness traverse, and the non-destructive testing reports referenced to the procedure used.